A 240 S30409 Stainless Steels to A 240/A 240M (2012)

A 240 S30409 - Specification & Application

  • A 240/A 240M (2012) - Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications

Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications

Chemical composition(wt.%) of A 240 S30409 grade: to A 240/A 240M (2012)

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.04 0.10
Si - 1.00
Mn - 2.00
P - 0.04
S - 0.03
Cr 18.0 20.0
Ni 8.00 11.0

A 240 S30409 - Detail

Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications

Mechanical properties of grade A 240 S30409 A 240/A 240M (2012)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
249 (≥) 374 (≥) 13 41 44 Solution and Aging, Annealing, Ausaging, Q+T,etc 421

Physical properties of grade A 240 S30409 A 240/A 240M (2012)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
357 (≥) 224 (≥) 22 44 32 Solution and Aging, Annealing, Ausaging, Q+T,etc 423
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
999 876 972