A 213 S32615 Stainless Steels to A 213/A 213M (2013)

A 213 S32615 - Specification & Application

  • A 213/A 213M (2013) - Seamless Ferritic and Austenitic Alloy-Steel Boiler, Superheater, and Heat-Exchanger Tubes

Seamless Ferritic and Austenitic Alloy-Steel Boiler, Superheater, and Heat-Exchanger Tubes

Chemical composition(wt.%) of A 213 S32615 grade: to A 213/A 213M (2013)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.06
Si - 0.75
Mn - 0.75
P - -
S - -
Ni - 0.50
Cr 25.00 27.00
Al - -
Cu - 0.20
Ti - -
Fe - -
N - 0.04
Mo 0.75 1.50

A 213 S32615 - Detail

Seamless Ferritic and Austenitic Alloy-Steel Boiler, Superheater, and Heat-Exchanger Tubes

Mechanical properties of grade A 213 S32615 A 213/A 213M (2013)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
555 (≥) 272 (≥) 42 24 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 414

Physical properties of grade A 213 S32615 A 213/A 213M (2013)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
881 (≥) 863 (≥) 34 11 34 Solution and Aging, Annealing, Ausaging, Q+T,etc 113
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
486 534 344