09X15H8Ю Stainless Steels

09X15H8Ю - Specification & Application

Russia GOCT standard stainless steel and heat resistant steel steel grade and chemical composition

Chemical composition(wt.%) of 09X15H8Ю grade:

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.90
Si - 0.80
Mn - 0.80
P - 0.035
S - 0.025
Cr 14.00 16.00
Ni 7.00 9.40
Mo - 0.30
W - 0.20
Ti - 0.20
Al 0.70 1.30

09X15H8Ю - Detail

Russia GOCT standard stainless steel and heat resistant steel steel grade and chemical composition

Mechanical properties of grade 09X15H8Ю

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
375 (≥) 166 (≥) 24 41 44 Solution and Aging, Annealing, Ausaging, Q+T,etc 433

Physical properties of grade 09X15H8Ю

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
181 (≥) 637 (≥) 43 41 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 112
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
215 896 782

Equivalent Grade

Equivalent Products

We can customize the production of 09X15H8Ю grade, contact us for the best solution.