X6CrNiTi18-10 Stainless Steels to ISO 15510 (2010)

X6CrNiTi18-10 - Specification & Application

  • ISO 15510 (2010) - Stainless steels -- Chemical composition
  • ISO 16143-1 (2004) - Stainless steels for general purposes -- Part 1: Flat products
  • ISO 16143-2 (2004) - Stainless steels for general purposes -- Part 2: Semi-finished products, bars, rods and sections
  • ISO 16143-3 (2005) - Stainless steels for general purposes -- Part 3: Wire
  • ISO 9327-5 (1999) - Steel forgings and rolled or forged bars for pressure purposes - Technical delivery conditions - Part 5: Stainless steels
  • ISO 9328-5 - Steel plates and strips for pressure purposes - Technical delivery conditions - Part 5: Weldable fine grain steels, thermomechanically rolled
  • ISO 9328-7 (2011) - Steel flat products for pressure purposes - Technical delivery conditions - Part 7: Stainless steels
  • ISO 9329-4 (1997) - Seamless steel tubes for pressure purposes - Technical delivery conditions - Part 4: Austenitic stainless steels
  • ISO 9330-6 (1997) - Welded steel tubes for pressure purposes - Technical delivery conditions - Part 6: Longitudinally welded austenitic stainless steel tubes
  • ISO/TS 15510 (2003) - Welded steel tubes for pressure purposes - Technical delivery conditions - Part 6: Longitudinally welded austenitic stainless steel tubes

Welded steel tubes for pressure purposes - Technical delivery conditions - Part 6: Longitudinally welded austenitic stainless steel tubes

Chemical composition(wt.%) of X6CrNiTi18-10 grade: to ISO 15510 (2010)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.08
Si - 1.00
Mn - 2.00
P - 0.040
S - 0.030
Cr 17.00 19.00
Mo 9.00 12.00
Ni - -

X6CrNiTi18-10 - Detail

Welded steel tubes for pressure purposes - Technical delivery conditions - Part 6: Longitudinally welded austenitic stainless steel tubes

Mechanical properties of grade X6CrNiTi18-10 ISO 15510 (2010)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
721 (≥) 471 (≥) 12 42 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 423

Physical properties of grade X6CrNiTi18-10 ISO 15510 (2010)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
979 (≥) 616 (≥) 31 33 13 Solution and Aging, Annealing, Ausaging, Q+T,etc 411
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
356 117 531

Equivalent Products

We can customize the production of X6CrNiTi18-10 grade, contact us for the best solution.