Welded steel tubes for pressure purposes - Technical delivery conditions - Part 6: Longitudinally welded austenitic stainless steel tubes
Elements | Min.(≥) | Max.(≤) | Similar | Remarks |
---|---|---|---|---|
C | 0.04 | 0.07 | ||
Si | - | 1.00 | ||
Mn | - | 2.00 | ||
P | - | 0.040 | ||
S | - | 0.030 | ||
Cr | 17.00 | 19.00 | ||
Mo | 8.00 | 11.00 | ||
Ni | - | - |
Welded steel tubes for pressure purposes - Technical delivery conditions - Part 6: Longitudinally welded austenitic stainless steel tubes
Proof strength Rp0.2 (MPa) |
Tensile strength Rm (MPa) |
Impact energy KV (J) |
Elongation at fracture A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
438 (≥) | 916 (≥) | 44 | 12 | 13 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 342 |
Property | Density kg/dm3 |
Temperature T °C/F |
Specific heat J / kgK |
Thermal conductivity W/mK |
Electric resistance µΩ·cm |
Modulus of elasticity kN/mm2 |
Expansion rate |
---|---|---|---|---|---|---|---|
682 (≥) | 635 (≥) | 23 | 34 | 44 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 124 | |
Temp. °C/°F |
Creep strain limit (10000h) (Rp1,0) N/mm2 |
Creep rupture strength (10000h) (Rp1,0) N/mm2 |
|||||
155 | 653 | 681 |
We can customize the production of X7CrNi18-9 grade, contact us for the best solution.