SUS 309S Stainless Steels to G 4311 (2011)

SUS 309S - Specification & Application

  • G 4311 (2011) - Heat-resisting steel bars and wire rods

Heat-resisting steel bars and wire rods

Chemical composition(wt.%) of SUS 309S grade: to G 4311 (2011)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.08
Si - 1.00
Mn - 2.00
P - 0.045
S - 0.03
Cr 22.00 24.00
Ni 12.00 15.00
Mo - -
N - -

SUS 309S - Detail

Heat-resisting steel bars and wire rods

Mechanical properties of grade SUS 309S G 4311 (2011)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
374 (≥) 462 (≥) 33 43 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 433

Physical properties of grade SUS 309S G 4311 (2011)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
775 (≥) 598 (≥) 21 41 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 121
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
438 588 711

Equivalent Products

We can customize the production of SUS 309S grade, contact us for the best solution.