STS329J4LTB Stainless Steels to D 3577 (2007)

STS329J4LTB - Specification & Application

  • D 3577 (2007) - Stainless steel for boiler and heat exchanger tubes

Stainless steel for boiler and heat exchanger tubes

Chemical composition(wt.%) of STS329J4LTB grade: to D 3577 (2007)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.03
Si - 1.00
Mn - 1.50
P - 0.040
S - 0.030
Cr 24.00 26.00
Ni 5.50 7.50
Mo 2.50 3.50
N 0.08 0.30

STS329J4LTB - Detail

Stainless steel for boiler and heat exchanger tubes

Mechanical properties of grade STS329J4LTB D 3577 (2007)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
949 (≥) 281 (≥) 43 22 12 Solution and Aging, Annealing, Ausaging, Q+T,etc 414

Physical properties of grade STS329J4LTB D 3577 (2007)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
952 (≥) 255 (≥) 41 32 11 Solution and Aging, Annealing, Ausaging, Q+T,etc 242
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
731 396 674

Equivalent Products

We can customize the production of STS329J4LTB grade, contact us for the best solution.