SUS 420F Stainless Steels to G 4318 (2007)

SUS 420F - Specification & Application

  • G 4318 (2007) - Cold finished stainless steel bars

Cold finished stainless steel bars

Chemical composition(wt.%) of SUS 420F grade: to G 4318 (2007)

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.26 0.40
Si - 1.00
Mn - 1.00
P - 0.06
S - 0.15
Cr 12.00 14.00
Ni - 0.60
Mo - 0.60
N - -

SUS 420F - Detail

Cold finished stainless steel bars

Mechanical properties of grade SUS 420F G 4318 (2007)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
859 (≥) 994 (≥) 41 12 42 Solution and Aging, Annealing, Ausaging, Q+T,etc 442

Physical properties of grade SUS 420F G 4318 (2007)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
499 (≥) 677 (≥) 21 31 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 431
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
349 553 278

Equivalent Products

We can customize the production of SUS 420F grade, contact us for the best solution.
sales@specificsteel.com