A 693 Type XM-9 Stainless Steels to A 693 (2006)

A 693 Type XM-9 - Specification & Application

  • A 693 (2006) - Precipitation-Hardening Stainless and Heat-Resisting Steel Plate, Sheet, and Strip

Precipitation-Hardening Stainless and Heat-Resisting Steel Plate, Sheet, and Strip

Chemical composition(wt.%) of A 693 Type XM-9 grade: to A 693 (2006)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.50
Mn - 0.50
Si - 0.30
P - 0.03
S - 0.03
Cr 14.00 15.00
Ni 6.00 7.00
Mo - -
Al - 0.10
Ti 0.60 0.90

A 693 Type XM-9 - Detail

Specification for Precipitation-Hardening Stainless and Heat-Resisting Steel Plate, Sheet, and Strip

Mechanical properties of grade A 693 Type XM-9 A 693 (2006)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
672 (≥) 255 (≥) 14 32 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 224

Physical properties of grade A 693 Type XM-9 A 693 (2006)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
151 (≥) 259 (≥) 33 14 14 Solution and Aging, Annealing, Ausaging, Q+T,etc 241
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
213 151 668

Equivalent Products

We can customize the production of A 693 Type XM-9 grade, contact us for the best solution.
sales@specificsteel.com