CW-3 Special Alloy

Chemical composition%of the ladle analysis of gradeCW-3

C(%)W(%)Co(%)Nb(%)Ti(%)Ta(%)
6.872.26.72.34.97.0
CW-3
Density / (g/cm ^ 3) : 12.45 Hardness HRC: 92.0 σ bb/MPa: 1760 Grain size/μ m: 2 ~ 3 and 6 Use for example: used for molding tool and the tip of a lot of arc radius cutting tools, cutting steel

Mechanical properties of gradeCW-3

Proof strength
Rp0.2(MPa)
Tensile strength
Rm(MPa)
Impact energy
KV(J)
Elongation at fracture
A(%)
Reduction in cross section on fracture
Z(%)
As-Heat-Treated Condition Brinell hardness(HBW)
576(≥) 928(≥) 31 31 14 Solution and Aging,Annealing,Ausaging,Q+T,etc 334

Physical properties of grade CW-3

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J/kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
797(≥) 457(≥) 23 42 44 Solution and Aging,Annealing,Ausaging,Q+T,etc 441
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0)N/mm2
Creep rupture strength
(10000h)
(Rp1,0)N/mm2
523 641 222

CW-3 Range of products

Product type Products Dimension Processes Deliver Status
Plates/Sheets Plates/Sheets 0.08-200mm(T)*W*L Forging,hot rolling and cold rolling Annealed,Solution and Aging,Q+T,ACID-WASHED,Shot Blasting
Steel Bar Round Bar,Flat Bar,Square Bar Φ8-1200mm*L Forging,hot rolling and cold rolling,Cast Black,Rough Turning,Shot Blasting,
Coil/Strip Steel Coil/Steel Strip 0.03-16.0x1200mm Cold-Rolled&Hot-Rolled Annealed,Solution and Aging,Q+T,ACID-WASHED,Shot Blasting
Pipes/Tubes Seamless Pipes/Tubes,Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion,Cold Drawn,Welded Annealed,Solution and Aging,Q+T,ACID-WASHED