SUS F 304LN Stainless Steels to G 3214 (2009)

SUS F 304LN - Specification & Application

  • G 3214 (2009) - Stainless steel forgings for pressure vessels

Stainless steel forgings for pressure vessels

Chemical composition(wt.%) of SUS F 304LN grade: to G 3214 (2009)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.03
Si - 1.00
Mn - 2.00
P - 0.045
S - 0.03
Cr 18.0 20.0
Ni 8.00 12.0
N 0.10 0.16

SUS F 304LN - Detail

Stainless steel forgings for pressure vessels

Mechanical properties of grade SUS F 304LN G 3214 (2009)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
214 (≥) 337 (≥) 22 44 44 Solution and Aging, Annealing, Ausaging, Q+T,etc 413

Physical properties of grade SUS F 304LN G 3214 (2009)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
327 (≥) 214 (≥) 12 22 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 124
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
479 952 375

Equivalent Products

We can customize the production of SUS F 304LN grade, contact us for the best solution.