Chemical composition(wt.%) of X38CrMoV15 grade: to DIN 17442 (1977)

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.35 0.40
Si - 1.00
Mn - 1.00
P - 0.040
S - 0.030
Cr 14.0 15.0
Mo 0.40 0.60
V 0.10 0.15

X38CrMoV15 - Detail

Rolled, Wrought or Cast Stainless Steel Products for Medical Instruments

Mechanical properties of grade X38CrMoV15 DIN 17442 (1977)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
536 (≥) 453 (≥) 34 34 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 114

Physical properties of grade X38CrMoV15 DIN 17442 (1977)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
575 (≥) 739 (≥) 11 13 12 Solution and Aging, Annealing, Ausaging, Q+T,etc 432
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
469 689 461