XM-5 Stainless Steels to ASTM A 581 / A 581M

XM-5 - Specification & Application

  • ASTM A 581 / A 581M - Free machining stainless and heat resisting steel wire
  • ASTM A 582/A 582M - Free-machining stainless steel bars

Free machining stainless and heat resisting steel wire

Chemical composition(wt.%) of XM-5 grade: to ASTM A 581 / A 581M

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.15
Si - 1.00
Mn 2.50 4.50
P - 0.2
S 0.15 -
Cr 17.0 19.0
Ni 7.00 10.0
Mo - 0.60

XM-5 - Detail

Free machining stainless and heat resisting steel wire

Mechanical properties of grade XM-5 ASTM A 581 / A 581M

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
345 (≥) 438 (≥) 32 32 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 343

Physical properties of grade XM-5 ASTM A 581 / A 581M

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
177 (≥) 632 (≥) 32 43 32 Solution and Aging, Annealing, Ausaging, Q+T,etc 441
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
921 927 578

Equivalent Products

We can customize the production of XM-5 grade, contact us for the best solution.
sales@specificsteel.com