81MoCrV42-16 Tool Die Steels to DIN 17230 (1980)

81MoCrV42-16 - Specification & Application

  • DIN 17230 (1980) - Ball and Roller Bearing Steels; Technical Conditions of Delivery

Ball and Roller Bearing Steels; Technical Conditions of Delivery

Chemical composition(wt.%) of 81MoCrV42-16 grade: to DIN 17230 (1980)

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.77 1.85
Si - 0.25
Mn - 0.35
P - -
S - -
Cr 3.75 4.25
Mo 4.00 4.50
V 0.90 1.10

81MoCrV42-16 - Detail

Ball and Roller Bearing Steels; Technical Conditions of Delivery

Mechanical properties of grade 81MoCrV42-16 DIN 17230 (1980)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
958 (≥) 967 (≥) 43 22 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 341

Physical properties of grade 81MoCrV42-16 DIN 17230 (1980)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
798 (≥) 764 (≥) 12 12 31 Solution and Aging, Annealing, Ausaging, Q+T,etc 314
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
723 559 194

Equivalent Grade

Equivalent Products

We can customize the production of 81MoCrV42-16 grade, contact us for the best solution.