00Cr18Mo2 Stainless Steels to GB/T 12771 (2000)

00Cr18Mo2 - Specification & Application

  • GB/T 12771 (2000) - Welded stainless steel pipes for liquid delivery
  • GB/T 3280 (2007) - Cold rolled stainless steel sheets and plates
  • GB/T 4237 (1992) - Hot rolled stainless steel sheets and plates
  • GB/T 4239 (1991) - Cold rolled stainless steel and heat resisting steel strips

Welded stainless steel pipes for liquid delivery

Chemical composition(wt.%) of 00Cr18Mo2 grade: to GB/T 12771 (2000)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.025
Si - 1.00
Mn - 1.00
P - 0.035
S - 0.030
Ni - 0.60
Cr 17.00 20.00
Mo 1.75 2.50

00Cr18Mo2 - Detail

00Cr18Mo2

Mechanical properties of grade 00Cr18Mo2 GB/T 12771 (2000)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
928 (≥) 844 (≥) 41 32 31 Solution and Aging, Annealing, Ausaging, Q+T,etc 334

Physical properties of grade 00Cr18Mo2 GB/T 12771 (2000)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
778 (≥) 275 (≥) 24 23 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 134
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
988 224 482

Equivalent Grade

Equivalent Products

We can customize the production of 00Cr18Mo2 grade, contact us for the best solution.