301 Stainless Steels to A 240/A 240M (2012)

301 - Specification & Application

  • A 240/A 240M (2012) - Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications
  • A 554 (2011) - Welded Stainless Steel Mechanical Tubing
  • A 666 (2010) - Annealed or Cold-Worked Austenitic Stainless Steel Sheet, Strip, Plate, and Flat Bar
  • A 959 (2011) - Standard Guide for Specifying Harmonized Standard Grade Compositions for Wrought Stainless Steels
  • SAE J 405 (1998) - Chemical compositions of SAE wrought stainless steels

Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications

Chemical composition(wt.%) of 301 grade: to A 240/A 240M (2012)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.15
Si - 1.00
Mn - 2.00
P - 0.045
S - 0.03
Cr 16.0 18.0
Ni 6.00 8.00

301 - Detail

AISI 301

Mechanical properties of grade 301 A 240/A 240M (2012)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
186 (≥) 644 (≥) 12 21 34 Solution and Aging, Annealing, Ausaging, Q+T,etc 422

Physical properties of grade 301 A 240/A 240M (2012)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
324 (≥) 499 (≥) 21 42 44 Solution and Aging, Annealing, Ausaging, Q+T,etc 133
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
721 127 181
We can customize the production of 301 grade, contact us for the best solution.
sales@specificsteel.com