35B2 Stainless Steels to NF EN 10269

35B2 - Specification & Application

  • NF EN 10269 - Steels and nickel alloys for fasteners with specified elevated and/or low temperature properties

Steels and nickel alloys for fasteners with specified elevated and/or low temperature properties

Chemical composition(wt.%) of 35B2 grade: to NF EN 10269

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.32 0.39
Si - 0.40
Mn 0.50 0.80
P - 0.035
S - 0.035
Cr - -
Ni - -
Mo - -
Al - 0.020
B 0.0008 0.0050

35B2 - Detail

Steels and nickel alloys for fasteners with specified elevated and/or low temperature properties

Mechanical properties of grade 35B2 NF EN 10269

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
168 (≥) 894 (≥) 41 23 11 Solution and Aging, Annealing, Ausaging, Q+T,etc 213

Physical properties of grade 35B2 NF EN 10269

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
437 (≥) 141 (≥) 12 33 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 434
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
824 641 878

Equivalent Grade

Equivalent Products

We can customize the production of 35B2 grade, contact us for the best solution.