54NiCrMoV6 Tool Die Steels

54NiCrMoV6 - Specification & Application

Alloyed NiCrMoV steel

Chemical composition(wt.%) of 54NiCrMoV6 grade:

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.50 0.60
Si 0.15 0.35
Mn 0.50 0.80
P - 0.025
S - 0.035
Cr 0.60 0.80
Mo 0.25 0.35
V 0.08 0.12
Ni 1.50 1.80

54NiCrMoV6 - Detail

Alloyed NiCrMoV steel

Mechanical properties of grade 54NiCrMoV6

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
282 (≥) 233 (≥) 32 23 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 123

Physical properties of grade 54NiCrMoV6

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
441 (≥) 441 (≥) 43 21 31 Solution and Aging, Annealing, Ausaging, Q+T,etc 412
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
296 231 186

Equivalent Grade

Equivalent Products

We can customize the production of 54NiCrMoV6 grade, contact us for the best solution.
sales@specificsteel.com