A 1082 S32950 Stainless Steels to A1082/A1082M (2012)

A 1082 S32950 - Specification & Application

  • A1082/A1082M (2012) - High Strength Precipitation Hardening and Duplex Stainless Steel Bolting for Special Purpose Applications

High Strength Precipitation Hardening and Duplex Stainless Steel Bolting for Special Purpose Applications

Chemical composition(wt.%) of A 1082 S32950 grade: to A1082/A1082M (2012)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.03
Mn - 2.00
Si - 0.60
P - 0.035
S - 0.01
Cr 26.00 29.00
Ni 3.50 5.20
Mo 1.00 2.50
N 0.15 0.25

A 1082 S32950 - Detail

High Strength Precipitation Hardening and Duplex Stainless Steel Bolting for Special Purpose Applications

Mechanical properties of grade A 1082 S32950 A1082/A1082M (2012)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
253 (≥) 675 (≥) 34 42 24 Solution and Aging, Annealing, Ausaging, Q+T,etc 314

Physical properties of grade A 1082 S32950 A1082/A1082M (2012)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
184 (≥) 398 (≥) 31 11 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 311
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
623 668 414

Equivalent Products

We can customize the production of A 1082 S32950 grade, contact us for the best solution.