A 249 S30403 Stainless Steels to A 249/A 249M (2010)

A 249 S30403 - Specification & Application

  • A 249/A 249M (2010) - Welded Austenitic Steel Boiler, Superheater, Heat-Exchanger, and Condenser Tubes

Welded Austenitic Steel Boiler, Superheater, Heat-Exchanger, and Condenser Tubes

Chemical composition(wt.%) of A 249 S30403 grade: to A 249/A 249M (2010)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.03
Si - 1.00
Mn - 2.00
P - 0.045
S - 0.03
Cr 18.0 20.0
Ni 8.00 12.0

A 249 S30403 - Detail

Welded Austenitic Steel Boiler, Superheater, Heat-Exchanger, and Condenser Tubes

Mechanical properties of grade A 249 S30403 A 249/A 249M (2010)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
156 (≥) 686 (≥) 32 44 42 Solution and Aging, Annealing, Ausaging, Q+T,etc 234

Physical properties of grade A 249 S30403 A 249/A 249M (2010)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
495 (≥) 155 (≥) 13 23 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 223
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
632 746 369
We can customize the production of A 249 S30403 grade, contact us for the best solution.