A 314 S43023 Stainless Steels to A 314 (2008)

A 314 S43023 - Specification & Application

  • A 314 (2008) - Stainless Steel Billets and Bars for Forging

Stainless Steel Billets and Bars for Forging

Chemical composition(wt.%) of A 314 S43023 grade: to A 314 (2008)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.12
Mn - 1.25
Si - 1.00
P - 0.06
S - 0.06
Cr 16.00 18.00
Ni - -
Mo - -
Se - 0.15

A 314 S43023 - Detail

Stainless Steel Billets and Bars for Forging

Mechanical properties of grade A 314 S43023 A 314 (2008)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
393 (≥) 249 (≥) 12 12 32 Solution and Aging, Annealing, Ausaging, Q+T,etc 312

Physical properties of grade A 314 S43023 A 314 (2008)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
759 (≥) 616 (≥) 33 23 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 332
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
573 133 112

Equivalent Products

We can customize the production of A 314 S43023 grade, contact us for the best solution.