S355J2WP Special Alloy

Chemical composition%of the ladle analysis of gradeS355J2WP

C(%)Si(%)Mn(%)P(%)S(%)Cr(%)Ni(%)Cu(%)
0.120.75Max 1.000.06-0.150.0350.30-1.250.650.25-0.55
S355J2WP

Mechanical properties of gradeS355J2WP

Proof strength
Rp0.2(MPa)
Tensile strength
Rm(MPa)
Impact energy
KV(J)
Elongation at fracture
A(%)
Reduction in cross section on fracture
Z(%)
As-Heat-Treated Condition Brinell hardness(HBW)
329(≥) 926(≥) 32 44 33 Solution and Aging,Annealing,Ausaging,Q+T,etc 341

Physical properties of grade S355J2WP

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J/kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
484(≥) 868(≥) 34 14 44 Solution and Aging,Annealing,Ausaging,Q+T,etc 443
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0)N/mm2
Creep rupture strength
(10000h)
(Rp1,0)N/mm2
784 173 183

S355J2WP Range of products

Product type Products Dimension Processes Deliver Status
Plates/Sheets Plates/Sheets 0.08-200mm(T)*W*L Forging,hot rolling and cold rolling Annealed,Solution and Aging,Q+T,ACID-WASHED,Shot Blasting
Steel Bar Round Bar,Flat Bar,Square Bar Φ8-1200mm*L Forging,hot rolling and cold rolling,Cast Black,Rough Turning,Shot Blasting,
Coil/Strip Steel Coil/Steel Strip 0.03-16.0x1200mm Cold-Rolled&Hot-Rolled Annealed,Solution and Aging,Q+T,ACID-WASHED,Shot Blasting
Pipes/Tubes Seamless Pipes/Tubes,Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion,Cold Drawn,Welded Annealed,Solution and Aging,Q+T,ACID-WASHED

Equivalent Grade