T30102 Tool Die Steels

T30102 - Specification & Application

Cold-Work Tool Steel

Chemical composition(wt.%) of T30102 grade:

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.95 1.05
Si 0.10 0.50
Mn 0.40 1.00
P - 0.030
S - 0.030
Cr 4.75 5.50
Mo 0.90 1.40
V 0.15 0.50
W - -
Ni+Cu - 0.75

T30102 - Detail

Cold-Work Tool Steel

Mechanical properties of grade T30102

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
696 (≥) 992 (≥) 31 12 14 Solution and Aging, Annealing, Ausaging, Q+T,etc 313

Physical properties of grade T30102

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
398 (≥) 337 (≥) 32 14 12 Solution and Aging, Annealing, Ausaging, Q+T,etc 212
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
852 937 169

Equivalent Grade

Equivalent Products

We can customize the production of T30102 grade, contact us for the best solution.