X2CrMoTi18-2 Stainless Steels to NF EN 10028-7

X2CrMoTi18-2 - Specification & Application

  • NF EN 10028-7 - Flat products made of steels for pressure purposes - Part 7: Stainless steels
  • NF EN 10088-1 - Stainless steels - Part 1: List of stainless steels
  • NF EN 10088-2 - Stainless steels - Part 2: Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
  • NF EN 10088-4 - Stainless steels - Part 4: Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for construction purposes
  • NF EN 10296-2 (2005) - Welded circular steel tubes for mechanical and general engineering purposes - Technical delivery conditions - Part 2: Stainless steel

Welded circular steel tubes for mechanical and general engineering purposes - Technical delivery conditions - Part 2: Stainless steel

Chemical composition(wt.%) of X2CrMoTi18-2 grade: to NF EN 10028-7

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.025
Si - 1.00
Mn - 1.00
P - 0.040
S - 0.015
Cr 17.00 20.00
Mo 1.80 2.50
Ni - -
Ti 12×(C+N)+0.15 0.80
N - 0.030

X2CrMoTi18-2 - Detail

Welded circular steel tubes for mechanical and general engineering purposes - Technical delivery conditions - Part 2: Stainless steel

Mechanical properties of grade X2CrMoTi18-2 NF EN 10028-7

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
317 (≥) 622 (≥) 11 23 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 142

Physical properties of grade X2CrMoTi18-2 NF EN 10028-7

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
998 (≥) 179 (≥) 32 13 11 Solution and Aging, Annealing, Ausaging, Q+T,etc 411
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
987 979 683