X5CrNiMoCuNb14-5 Stainless Steels to BS EN 10088-1

X5CrNiMoCuNb14-5 - Specification & Application

  • BS EN 10088-1 - Stainless steels - Part 1: List of stainless steels
  • BS EN 10088-3 - Stainless steels - Part 3: Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes

Stainless steels - Part 3: Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes

Chemical composition(wt.%) of X5CrNiMoCuNb14-5 grade: to BS EN 10088-1

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.07
Si - 0.70
Mn - 1.00
P - 0.04
S - 0.015
Cr 13.00 15.00
Ni 5.00 6.00
Mo 1.20 2.00
Nb+Ta 0.15 0.60
Cu 1.20 2.00

X5CrNiMoCuNb14-5 - Detail

Stainless steels - Part 3: Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes

Mechanical properties of grade X5CrNiMoCuNb14-5 BS EN 10088-1

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
554 (≥) 287 (≥) 12 31 42 Solution and Aging, Annealing, Ausaging, Q+T,etc 443

Physical properties of grade X5CrNiMoCuNb14-5 BS EN 10088-1

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
377 (≥) 948 (≥) 13 23 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 124
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
314 163 786

Equivalent Products

We can customize the production of X5CrNiMoCuNb14-5 grade, contact us for the best solution.
sales@specificsteel.com