Z3CND22-05Az Stainless Steels to NF A 35-573

Z3CND22-05Az - Specification & Application

  • NF A 35-573 - Stainless steels for general purposes. Plates, wide strips and strips
  • NF A 35-574 - Iron and steel. Stainless steel for general purposes. Semi- finished products, bars and wire rod
  • NF A 36-209 - Iron and steel. Austenitic and austenic-ferritic stainless steels plates for boilers and pressure vessels
  • NF A 49-244 - Steel tubes - Welded austenitic stainless and austenitic ferritic steel rolled tubes for pressure service - Dimensions, technical conditions for delivery

Steel tubes - Welded austenitic stainless and austenitic ferritic steel rolled tubes for pressure service - Dimensions, technical conditions for delivery

Chemical composition(wt.%) of Z3CND22-05Az grade: to NF A 35-573

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.030
Si - 0.75
Mn - 2.00
P - 0.035
S - 0.010
Cr 21.00 23.00
Mo 2.50 3.50
Ni 4.50 6.50
N 0.08 0.20

Z3CND22-05Az - Detail

Steel tubes - Welded austenitic stainless and austenitic ferritic steel rolled tubes for pressure service - Dimensions, technical conditions for delivery

Mechanical properties of grade Z3CND22-05Az NF A 35-573

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
369 (≥) 914 (≥) 42 13 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 131

Physical properties of grade Z3CND22-05Az NF A 35-573

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
868 (≥) 513 (≥) 42 32 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 444
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
765 197 989

Equivalent Grade

Equivalent Products

We can customize the production of Z3CND22-05Az grade, contact us for the best solution.
sales@specificsteel.com