NiCr23Mo16Al Superalloys to DIN EN 17744

NiCr23Mo16Al - Specification & Application

  • DIN EN 17744 - The chemically stable and high-temperature resistant nickel and cobalt alloy 2.4605 (alloy 59) is mainly used in the chemical industry, flue gas desulphurating plants, paper industry.

The chemically stable and high-temperature resistant nickel and cobalt alloy 2.4605 (alloy 59) is mainly used in the chemical industry, flue gas desulphurating plants, paper industry.

Chemical composition(wt.%) of NiCr23Mo16Al grade: to DIN EN 17744

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.01
Si - 0.10
Mn - 0.50
P - 0.025
S - 0.015
Cr 22.00 24.00
Ni - Bal
Al 0.10 0.40
Co - 0.30
Cu - 0.50
Fe - 1.50

NiCr23Mo16Al - Detail

The chemically stable and high-temperature resistant nickel and cobalt NiCr23Mo16Al is mainly used in the chemical industry, flue gas desulphurating plants, paper industry.
Our product range in NiCr23Mo16Al are tubes and pipes, fittings and flanges, accessories.

Mechanical properties of grade NiCr23Mo16Al DIN EN 17744

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
254 (≥) 468 (≥) 34 41 43 Solution and Aging, Annealing, Ausaging, Q+T,etc 133

Physical properties of grade NiCr23Mo16Al DIN EN 17744

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
669 (≥) 383 (≥) 23 12 42 Solution and Aging, Annealing, Ausaging, Q+T,etc 312
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
763 796 416

Equivalent Products

We can customize the production of NiCr23Mo16Al grade, contact us for the best solution.