X 19 CrMoVNbN 11 1 Stainless Steels to DIN 17240 (1976)

X 19 CrMoVNbN 11 1 - Specification & Application

  • DIN 17240 (1976) - Heat Resisting and Highly Heat Resisting Materials for Bolts and Nuts; Quality Specifications

Heat Resisting and Highly Heat Resisting Materials for Bolts and Nuts; Quality Specifications

Chemical composition(wt.%) of X 19 CrMoVNbN 11 1 grade: to DIN 17240 (1976)

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.1700 0.2300
Mn 0.4000 0.9000
P - 0.0250
S - 0.0150
Si - 0.5000
Ni 0.2000 0.6000
Cr 10.0000 11.5000
Mo 0.5000 0.8000
V 0.1000 0.3000
B - 0.0015
Al - 0.0200
N 0.0500 0.1000
Nb 0.2500 0.5500

X 19 CrMoVNbN 11 1 - Detail

Heat Resisting and Highly Heat Resisting Materials for Bolts and Nuts; Quality Specifications

Mechanical properties of grade X 19 CrMoVNbN 11 1 DIN 17240 (1976)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
882 (≥) 968 (≥) 32 31 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 341

Physical properties of grade X 19 CrMoVNbN 11 1 DIN 17240 (1976)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
994 (≥) 933 (≥) 41 22 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 343
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
982 285 115