X6CrAl13 Stainless Steels to NF EN 10088-1

X6CrAl13 - Specification & Application

  • NF EN 10088-1 - Stainless steels - Part 1: List of stainless steels
  • NF EN 10088-2 - Stainless steels - Part 2: Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
  • NF EN 10250-4 - Open die steel forgings for general engineering purposes - Part 4: Stainless steels
  • NF EN 10297-2 (2005) - Seamless circular steel tubes for mechanical and general engineering purposes - Technical delivery conditions - Part 2: Stainless steel

Seamless circular steel tubes for mechanical and general engineering purposes - Technical delivery conditions - Part 2: Stainless steel

Chemical composition(wt.%) of X6CrAl13 grade: to NF EN 10088-1

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.080
Si - 1.00
Mn - 1.00
P - 0.040
S - 0.015
Cr 12.00 14.00
Mo - -
Ni - -
Al 0.10 0.30

X6CrAl13 - Detail

Seamless circular steel tubes for mechanical and general engineering purposes - Technical delivery conditions - Part 2: Stainless steel

Mechanical properties of grade X6CrAl13 NF EN 10088-1

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
925 (≥) 959 (≥) 22 43 32 Solution and Aging, Annealing, Ausaging, Q+T,etc 323

Physical properties of grade X6CrAl13 NF EN 10088-1

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
126 (≥) 154 (≥) 21 24 43 Solution and Aging, Annealing, Ausaging, Q+T,etc 444
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
172 917 293

Equivalent Products

We can customize the production of X6CrAl13 grade, contact us for the best solution.