Z3CMD22-05-04Az Stainless Steels to NF A 35-573

Z3CMD22-05-04Az - Specification & Application

  • NF A 35-573 - Stainless steels for general purposes. Plates, wide strips and strips

Stainless steels for general purposes. Plates, wide strips and strips

Chemical composition(wt.%) of Z3CMD22-05-04Az grade: to NF A 35-573

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.030
Si - 0.75
Mn 4.00 7.00
P - 0.030
S - 0.010
Cr 21.00 23.00
Mo 2.00 3.50
Ni 3.00 4.50
N 0.25 0.40

Z3CMD22-05-04Az - Detail

Stainless steels for general purposes. Plates, wide strips and strips

Mechanical properties of grade Z3CMD22-05-04Az NF A 35-573

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
134 (≥) 459 (≥) 33 11 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 124

Physical properties of grade Z3CMD22-05-04Az NF A 35-573

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
212 (≥) 527 (≥) 42 24 32 Solution and Aging, Annealing, Ausaging, Q+T,etc 244
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
838 759 652

Equivalent Products

We can customize the production of Z3CMD22-05-04Az grade, contact us for the best solution.