Russia TY standard grades and chemical compositions of the high temperature alloy castings
Elements | Min.(≥) | Max.(≤) | Similar | Remarks |
---|---|---|---|---|
C | 0.07 | 0.12 | ||
Cr | 11.00 | 14.00 | ||
Al | 4.00 | 4.80 | ||
Mo | 3.50 | 5.00 | ||
Ti | 2.50 | 3.20 | ||
Co | 5.00 | 10.00 | ||
W | 3.50 | 5.00 | ||
Ni | - | remaining | ||
Nb | - | - | ||
Fe | - | 2.00 | ||
B | 0.01 | 0.02 | ||
Ce | 0.01 | 0.02 | ||
V | - | - | ||
Zr | - | - | ||
Mn | - | 0.40 | ||
Si | - | 0.40 | ||
S | - | 0.010 | ||
P | - | 0.015 |
Russia TY standard grades and chemical compositions of the high temperature alloy castings
Proof strength Rp0.2 (MPa) |
Tensile strength Rm (MPa) |
Impact energy KV (J) |
Elongation at fracture A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
517 (≥) | 631 (≥) | 14 | 11 | 32 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 112 |
Property | Density kg/dm3 |
Temperature T °C/F |
Specific heat J / kgK |
Thermal conductivity W/mK |
Electric resistance µΩ·cm |
Modulus of elasticity kN/mm2 |
Expansion rate |
---|---|---|---|---|---|---|---|
924 (≥) | 828 (≥) | 21 | 24 | 34 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 223 | |
Temp. °C/°F |
Creep strain limit (10000h) (Rp1,0) N/mm2 |
Creep rupture strength (10000h) (Rp1,0) N/mm2 |
|||||
937 | 658 | 246 |
We can customize the production of ЖC3ЛK grade, contact us for the best solution.