A 955 S31803 Grade 60 Stainless Steels to A 955/A 955M (2012)

A 955 S31803 Grade 60 - Specification & Application

  • A 955/A 955M (2012) - Deformed and Plain Stainless-Steel Bars for Concrete Reinforcement

Deformed and Plain Stainless-Steel Bars for Concrete Reinforcement

Chemical composition(wt.%) of A 955 S31803 Grade 60 grade: to A 955/A 955M (2012)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.03
Mn - 2.00
Si - 1.00
P - 0.03
S - 0.02
Cr 21.00 23.00
Ni 4.50 6.50
Mo 2.50 3.50
N 0.08 0.20

A 955 S31803 Grade 60 - Detail

Deformed and Plain Stainless-Steel Bars for Concrete Reinforcement

Mechanical properties of grade A 955 S31803 Grade 60 A 955/A 955M (2012)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
424 (≥) 238 (≥) 42 21 43 Solution and Aging, Annealing, Ausaging, Q+T,etc 231

Physical properties of grade A 955 S31803 Grade 60 A 955/A 955M (2012)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
761 (≥) 425 (≥) 12 31 11 Solution and Aging, Annealing, Ausaging, Q+T,etc 323
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
434 136 241

Equivalent Products

We can customize the production of A 955 S31803 Grade 60 grade, contact us for the best solution.