Chemical composition(wt.%) of 05X13H6M2 grade:

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.05
Si - 0.80
Mn - 0.80
P - 0.035
S - 0.025
Cr 12.00 13.50
Ni 5.50 6.50
Mo 1.50 1.90
Al - 0.15
Nb - 0.20

05X13H6M2 - Detail

Russia GOCT standard stainless steel and heat resistant steel steel grade and chemical composition

Mechanical properties of grade 05X13H6M2

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
962 (≥) 114 (≥) 12 12 24 Solution and Aging, Annealing, Ausaging, Q+T,etc 222

Physical properties of grade 05X13H6M2

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
211 (≥) 671 (≥) 44 21 24 Solution and Aging, Annealing, Ausaging, Q+T,etc 423
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
545 776 659

Equivalent Grade

Equivalent Products

We can customize the production of 05X13H6M2 grade, contact us for the best solution.