A 580 S21400 Stainless Steels to A 580/A 580M (2012)

A 580 S21400 - Specification & Application

  • A 580/A 580M (2012) - Stainless Steel Wire

Stainless Steel Wire

Chemical composition(wt.%) of A 580 S21400 grade: to A 580/A 580M (2012)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.05
Si - 0.20
Mn - 0.50
P - -
S - -
Ni - remaining
Cr 15.00 17.00
Al 4.00 5.00
Cu - -
Ti - 0.50
Fe 2.00 4.00
N - -
Mo - 0.50
B - 0.006
Zr - 0.05

A 580 S21400 - Detail

Stainless Steel Wire

Mechanical properties of grade A 580 S21400 A 580/A 580M (2012)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
222 (≥) 494 (≥) 34 13 31 Solution and Aging, Annealing, Ausaging, Q+T,etc 113

Physical properties of grade A 580 S21400 A 580/A 580M (2012)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
866 (≥) 773 (≥) 33 24 32 Solution and Aging, Annealing, Ausaging, Q+T,etc 314
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
483 328 787

Equivalent Products

We can customize the production of A 580 S21400 grade, contact us for the best solution.