H11 Stainless Steels to SAE AMS 6487K (2012)

H11 - Specification & Application

  • SAE AMS 6487K (2012) - Steel, Bars, and Forgings 5.0Cr - 1.3Mo - 0.50V (0.38 - 0.43C) (H-11) Consumable Electrode Vacuum Melted

Steel, Bars, and Forgings 5.0Cr - 1.3Mo - 0.50V (0.38 - 0.43C) (H-11) Consumable Electrode Vacuum Melted

Chemical composition(wt.%) of H11 grade: to SAE AMS 6487K (2012)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.40
Si - 0.90
Mn - 0.30
P - -
S - -
Ni - -
Cr - 5.00
Al - -
Cu - -
Ti - -
Fe - remaining
Mo - 1.30
Co - -
V - 0.50

H11 - Detail

Steel, Bars, and Forgings 5.0Cr - 1.3Mo - 0.50V (0.38 - 0.43C) (H-11) Consumable Electrode Vacuum Melted

Mechanical properties of grade H11 SAE AMS 6487K (2012)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
776 (≥) 113 (≥) 12 41 31 Solution and Aging, Annealing, Ausaging, Q+T,etc 123

Physical properties of grade H11 SAE AMS 6487K (2012)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
332 (≥) 443 (≥) 32 31 43 Solution and Aging, Annealing, Ausaging, Q+T,etc 224
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
651 577 597

Equivalent Products

We can customize the production of H11 grade, contact us for the best solution.