Marage 250 Stainless Steels to SAE AMS 6501D (2007)

Marage 250 - Specification & Application

  • SAE AMS 6501D (2007) - Steel, Maraging, Welding Wire 18Ni - 8.0Co - 4.9Mo - 0.40Ti - 0.10Al Vacuum Induction Melted, Environment Controlled Packaging

Steel, Maraging, Welding Wire 18Ni - 8.0Co - 4.9Mo - 0.40Ti - 0.10Al Vacuum Induction Melted, Environment Controlled Packaging

Chemical composition(wt.%) of Marage 250 grade: to SAE AMS 6501D (2007)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.03
Si - 0.10
Mn - 0.10
Ni - 18.00
Cr - -
Al - 0.10
Cu - -
Ti - 0.40
Fe - -
Mo - 5.00
Co - 8.00

Marage 250 - Detail

Steel, Maraging, Welding Wire 18Ni - 8.0Co - 4.9Mo - 0.40Ti - 0.10Al Vacuum Induction Melted, Environment Controlled Packaging

Mechanical properties of grade Marage 250 SAE AMS 6501D (2007)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
286 (≥) 937 (≥) 11 13 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 331

Physical properties of grade Marage 250 SAE AMS 6501D (2007)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
926 (≥) 743 (≥) 23 22 43 Solution and Aging, Annealing, Ausaging, Q+T,etc 422
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
938 363 581

Equivalent Products

We can customize the production of Marage 250 grade, contact us for the best solution.