S.127 Stainless Steels to BS S 127

S.127 - Specification & Application

  • BS S 127 - Specification for aircraft material. 24/17 chromium-nickel heat-resisting steel (titanium stabilized) (35 tonf/sq in: limiting ruling section 6 in)

Specification for aircraft material. 24/17 chromium-nickel heat-resisting steel (titanium stabilized) (35 tonf/sq in: limiting ruling section 6 in)

Chemical composition(wt.%) of S.127 grade: to BS S 127

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.15
Si 0.20 1.00
Mn 0.50 2.00
P - 0.035
S - 0.025
Cr 23.00 26.00
Ni 16.00 19.00
Mo - -
Ti - 4×C

S.127 - Detail

Specification for aircraft material. 24/17 chromium-nickel heat-resisting steel (titanium stabilized) (35 tonf/sq in: limiting ruling section 6 in)

Mechanical properties of grade S.127 BS S 127

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
675 (≥) 712 (≥) 23 22 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 224

Physical properties of grade S.127 BS S 127

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
619 (≥) 318 (≥) 22 42 34 Solution and Aging, Annealing, Ausaging, Q+T,etc 214
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
963 413 991