VF 10 Stainless Steels to SAE J 775 (2004)

VF 10 - Specification & Application

  • SAE J 775 (2004) - Engine poppet valve information report

Engine poppet valve information report

Chemical composition(wt.%) of VF 10 grade: to SAE J 775 (2004)

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.10 0.20
Si 1.00 1.40
Mn 0.50 0.80
P - -
S - -
Ni 19.00 22.00
Cr 7.00 9.00
Al - -
Cu - -
Ti - -
Fe - -
Mo - -
Co - -

VF 10 - Detail

Engine poppet valve information report

Mechanical properties of grade VF 10 SAE J 775 (2004)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
761 (≥) 927 (≥) 11 43 41 Solution and Aging, Annealing, Ausaging, Q+T,etc 423

Physical properties of grade VF 10 SAE J 775 (2004)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
226 (≥) 595 (≥) 32 41 44 Solution and Aging, Annealing, Ausaging, Q+T,etc 221
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
636 786 515

Equivalent Products

We can customize the production of VF 10 grade, contact us for the best solution.