Z6CN19-09Az Stainless Steels to NF A 35-573

Z6CN19-09Az - Specification & Application

  • NF A 35-573 - Stainless steels for general purposes. Plates, wide strips and strips
  • NF A 36-209 - Iron and steel. Austenitic and austenic-ferritic stainless steels plates for boilers and pressure vessels
  • NF A 49-244 - Steel tubes - Welded austenitic stainless and austenitic ferritic steel rolled tubes for pressure service - Dimensions, technical conditions for delivery

Steel tubes - Welded austenitic stainless and austenitic ferritic steel rolled tubes for pressure service - Dimensions, technical conditions for delivery

Chemical composition(wt.%) of Z6CN19-09Az grade: to NF A 35-573

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.06
Si - 1.00
Mn - 2.00
P - 0.040
S - 0.030
Cr 18.00 20.00
Mo - -
Ni 8.00 10.00
N 0.12 0.20

Z6CN19-09Az - Detail

Steel tubes - Welded austenitic stainless and austenitic ferritic steel rolled tubes for pressure service - Dimensions, technical conditions for delivery

Mechanical properties of grade Z6CN19-09Az NF A 35-573

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
319 (≥) 734 (≥) 24 24 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 423

Physical properties of grade Z6CN19-09Az NF A 35-573

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
455 (≥) 638 (≥) 14 14 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 422
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
439 456 184

Equivalent Grade

Equivalent Products

We can customize the production of Z6CN19-09Az grade, contact us for the best solution.