Specification for chromium-nickel-molybdenum-vanadium heat-resisting steel sheet and strip (930-1130 MPa: maximum thickness 6 mm) (Cr 12, Ni 2.5, Mo 1.7, V 0.3)
Elements | Min.(≥) | Max.(≤) | Similar | Remarks |
---|---|---|---|---|
C | 0.08 | 0.16 | ||
Si | - | 0.35 | ||
Mn | 0.50 | 0.90 | ||
P | - | 0.030 | ||
S | - | 0.025 | ||
Cr | 11.00 | 12.50 | ||
Ni | 2.00 | 3.00 | ||
Mo | 1.50 | 2.00 | ||
Nb/Ti | - | - | ||
V | 0.25 | 0.40 | ||
N | 0.02 | 0.04 |
Specification for chromium-nickel-molybdenum-vanadium heat-resisting steel sheet and strip (930-1130 MPa: maximum thickness 6 mm) (Cr 12, Ni 2.5, Mo 1.7, V 0.3)
Proof strength Rp0.2 (MPa) |
Tensile strength Rm (MPa) |
Impact energy KV (J) |
Elongation at fracture A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
332 (≥) | 911 (≥) | 34 | 14 | 44 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 432 |
Property | Density kg/dm3 |
Temperature T °C/F |
Specific heat J / kgK |
Thermal conductivity W/mK |
Electric resistance µΩ·cm |
Modulus of elasticity kN/mm2 |
Expansion rate |
---|---|---|---|---|---|---|---|
584 (≥) | 325 (≥) | 14 | 24 | 32 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 111 | |
Temp. °C/°F |
Creep strain limit (10000h) (Rp1,0) N/mm2 |
Creep rupture strength (10000h) (Rp1,0) N/mm2 |
|||||
179 | 244 | 163 |
We can customize the production of S.538 grade, contact us for the best solution.