A 314 S30200 Stainless Steels to A 314 (2008)

A 314 S30200 - Specification & Application

  • A 314 (2008) - Stainless Steel Billets and Bars for Forging

Stainless Steel Billets and Bars for Forging

Chemical composition(wt.%) of A 314 S30200 grade: to A 314 (2008)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.15
Si - 1.00
Mn - 2.00
P - 0.045
S - 0.03
Cr 17.0 19.0
Ni 8.00 10.00

A 314 S30200 - Detail

A 314 S30200 Stainless Steel Spring Wire  
This specification covers austenitic and age-hardenable stainless steel round spring wire intended especially for the manufacture of springs.  

Mechanical properties of grade A 314 S30200 A 314 (2008)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
949 (≥) 537 (≥) 33 33 12 Solution and Aging, Annealing, Ausaging, Q+T,etc 223

Physical properties of grade A 314 S30200 A 314 (2008)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
812 (≥) 392 (≥) 21 23 21 Solution and Aging, Annealing, Ausaging, Q+T,etc 134
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
645 512 136

Equivalent Products

We can customize the production of A 314 S30200 grade, contact us for the best solution.