B 625 N08925 Stainless Steels to B 625 (2011)

B 625 N08925 - Specification & Application

  • B 625 (2011) - UNS N08925, UNS N08031, UNS N08932, UNS N08926, UNS N08354, and UNS R20033 Plate, Sheet, and Strip

UNS N08925, UNS N08031, UNS N08932, UNS N08926, UNS N08354, and UNS R20033 Plate, Sheet, and Strip

Chemical composition(wt.%) of B 625 N08925 grade: to B 625 (2011)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.02
Mn - 1.00
Si - 0.50
P - 0.045
S - 0.03
Cr 24.00 26.00
Ni 19.00 21.00
Mo 6.00 7.00
Cu 0.80 1.50
N 0.10 0.20

B 625 N08925 - Detail

UNS N08925, UNS N08031, UNS N08932, UNS N08926, UNS N08354, and UNS R20033 Plate, Sheet, and Strip

Mechanical properties of grade B 625 N08925 B 625 (2011)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
925 (≥) 643 (≥) 33 42 24 Solution and Aging, Annealing, Ausaging, Q+T,etc 431

Physical properties of grade B 625 N08925 B 625 (2011)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
989 (≥) 634 (≥) 44 34 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 134
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
491 595 121

Equivalent Products

We can customize the production of B 625 N08925 grade, contact us for the best solution.