Ni-Mo16Cr-15 Stainless Steels to NF A 54-401

Ni-Mo16Cr-15 - Specification & Application

  • NF A 54-401 - Nickel and nickel alloys. Nickel-molybdenum and nickel-molybdenum- chromium-alloys

Nickel and nickel alloys. Nickel-molybdenum and nickel-molybdenum- chromium-alloys

Chemical composition(wt.%) of Ni-Mo16Cr-15 grade: to NF A 54-401

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.02
Si - 0.05
Mn - 1.00
P - 0.030
S - 0.030
Cr 14.50 16.50
Ni - remaining
Mo 15.00 17.00
V - 0.35
Co - 2.50
W 3.00 4.50

Ni-Mo16Cr-15 - Detail

Nickel and nickel alloys. Nickel-molybdenum and nickel-molybdenum- chromium-alloys

Mechanical properties of grade Ni-Mo16Cr-15 NF A 54-401

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
589 (≥) 393 (≥) 32 21 23 Solution and Aging, Annealing, Ausaging, Q+T,etc 344

Physical properties of grade Ni-Mo16Cr-15 NF A 54-401

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
675 (≥) 692 (≥) 32 43 32 Solution and Aging, Annealing, Ausaging, Q+T,etc 322
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
185 796 546

Equivalent Products

We can customize the production of Ni-Mo16Cr-15 grade, contact us for the best solution.