Nonmagnetizable Steel X55MnCr18-5 / 18Mn-4Cr Stainless Steels to ASTM STP 903

Nonmagnetizable Steel X55MnCr18-5 / 18Mn-4Cr - Specification & Application

  • ASTM STP 903 - Nonmagnetizable Steel

Nonmagnetizable Steel

Chemical composition(wt.%) of Nonmagnetizable Steel X55MnCr18-5 / 18Mn-4Cr grade: to ASTM STP 903

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.55
Mn - 18
Cr - 4.5

Nonmagnetizable Steel X55MnCr18-5 / 18Mn-4Cr - Detail

X55MnCr18-5 X55MnCr18-4 18Mn-4Cr

Mechanical properties of grade Nonmagnetizable Steel X55MnCr18-5 / 18Mn-4Cr ASTM STP 903

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
636 (≥) 976 (≥) 44 13 12 Solution and Aging, Annealing, Ausaging, Q+T,etc 421

Physical properties of grade Nonmagnetizable Steel X55MnCr18-5 / 18Mn-4Cr ASTM STP 903

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
124 (≥) 149 (≥) 14 21 13 Solution and Aging, Annealing, Ausaging, Q+T,etc 113
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
795 642 629