SKH3 Special Alloy

Chemical composition%of the ladle analysis of gradeSKH3

C(%)Si(%)Mn(%)Cr(%)V(%)W(%)Co(%)
0.73-0.83Max 0.45Max 0.403.80-4.500.80-1.2017.00-19.004.50-5.50
SKH3

Mechanical properties of gradeSKH3

Proof strength
Rp0.2(MPa)
Tensile strength
Rm(MPa)
Impact energy
KV(J)
Elongation at fracture
A(%)
Reduction in cross section on fracture
Z(%)
As-Heat-Treated Condition Brinell hardness(HBW)
876(≥) 644(≥) 44 13 22 Solution and Aging,Annealing,Ausaging,Q+T,etc 221

Physical properties of grade SKH3

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J/kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
653(≥) 138(≥) 31 33 13 Solution and Aging,Annealing,Ausaging,Q+T,etc 142
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0)N/mm2
Creep rupture strength
(10000h)
(Rp1,0)N/mm2
365 415 414

SKH3 Range of products

Product type Products Dimension Processes Deliver Status
Plates/Sheets Plates/Sheets 0.08-200mm(T)*W*L Forging,hot rolling and cold rolling Annealed,Solution and Aging,Q+T,ACID-WASHED,Shot Blasting
Steel Bar Round Bar,Flat Bar,Square Bar Φ8-1200mm*L Forging,hot rolling and cold rolling,Cast Black,Rough Turning,Shot Blasting,
Coil/Strip Steel Coil/Steel Strip 0.03-16.0x1200mm Cold-Rolled&Hot-Rolled Annealed,Solution and Aging,Q+T,ACID-WASHED,Shot Blasting
Pipes/Tubes Seamless Pipes/Tubes,Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion,Cold Drawn,Welded Annealed,Solution and Aging,Q+T,ACID-WASHED

Equivalent Grade