STR38 Stainless Steels to D 3731 (2002)

STR38 - Specification & Application

  • D 3731 (2002) - Heat - resisting steel bars

Heat - resisting steel bars

Chemical composition(wt.%) of STR38 grade: to D 3731 (2002)

Elements Min.(≥) Max.(≤) Similar Remarks
C 0.25 0.35
Si - 1.00
Mn - 1.20
P 0.18 0.25
S - 0.030
Cr 19.00 21.00
Ni 10.00 12.00
Mo 1.80 2.50
N - -
B 0.001 0.010

STR38 - Detail

Heat - resisting steel bars

Mechanical properties of grade STR38 D 3731 (2002)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
136 (≥) 122 (≥) 22 44 24 Solution and Aging, Annealing, Ausaging, Q+T,etc 413

Physical properties of grade STR38 D 3731 (2002)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
112 (≥) 361 (≥) 14 44 31 Solution and Aging, Annealing, Ausaging, Q+T,etc 244
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
924 923 834

Equivalent Grade

Equivalent Products

We can customize the production of STR38 grade, contact us for the best solution.
sales@specificsteel.com