Z3CND18-12-02 Stainless Steels to NF A 35-574

Z3CND18-12-02 - Specification & Application

  • NF A 35-574 - Iron and steel. Stainless steel for general purposes. Semi- finished products, bars and wire rod

Iron and steel. Stainless steel for general purposes. Semi- finished products, bars and wire rod

Chemical composition(wt.%) of Z3CND18-12-02 grade: to NF A 35-574

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.030
Si - 0.75
Mn - 2.00
P - 0.040
S 0.015 0.030
Cr 16.50 18.50
Mo 2.00 2.50
Ni 10.00 13.00

Z3CND18-12-02 - Detail

Iron and steel. Stainless steel for general purposes. Semi- finished products, bars and wire rod

Mechanical properties of grade Z3CND18-12-02 NF A 35-574

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
523 (≥) 546 (≥) 14 42 13 Solution and Aging, Annealing, Ausaging, Q+T,etc 121

Physical properties of grade Z3CND18-12-02 NF A 35-574

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
748 (≥) 846 (≥) 32 31 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 222
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
936 665 129

Equivalent Grade

Equivalent Products

We can customize the production of Z3CND18-12-02 grade, contact us for the best solution.