PH 14-8 Mo Stainless Steels to SAE AMS 5603E

PH 14-8 Mo - Specification & Application

  • SAE AMS 5603E - Sheet and Strip 15Cr - 8,4Ni - 2,2Mo - 1,1Al, vac. Induct. Melted, Solution Heat Treated

Sheet and Strip 15Cr - 8,4Ni - 2,2Mo - 1,1Al, vac. Induct. Melted, Solution Heat Treated

Chemical composition(wt.%) of PH 14-8 Mo grade: to SAE AMS 5603E

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.05
Si - -
Mn - -
Cr 13.50 15.50
Ni 7.50 9.50
Mo 2.00 3.00
Co - -
W - -
Al 0.75 1.50
Cu - -
Ti - -
Fe - -

PH 14-8 Mo - Detail

Sheet and Strip 15Cr - 8,4Ni - 2,2Mo - 1,1Al, vac. Induct. Melted, Solution Heat Treated

Mechanical properties of grade PH 14-8 Mo SAE AMS 5603E

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
585 (≥) 713 (≥) 23 33 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 234

Physical properties of grade PH 14-8 Mo SAE AMS 5603E

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
336 (≥) 746 (≥) 32 12 43 Solution and Aging, Annealing, Ausaging, Q+T,etc 343
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
693 563 531