Marage 300 Stainless Steels to SAE AMS 6514H (2012)

Marage 300 - Specification & Application

  • SAE AMS 6514H (2012) - Steel, Maraging, Bars, Forgings, Tubing, and Rings 18.5Ni - 9.0Co - 4.9Mo - 0.65Ti - 0.10Al Consumable Electrode Vacuum Melted, Annealed

Steel, Maraging, Bars, Forgings, Tubing, and Rings 18.5Ni - 9.0Co - 4.9Mo - 0.65Ti - 0.10Al Consumable Electrode Vacuum Melted, Annealed

Chemical composition(wt.%) of Marage 300 grade: to SAE AMS 6514H (2012)

Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.03
Si - 0.10
Mn - 0.10
Ni - 18.00
Cr - -
Al - 0.10
Cu - -
Ti - 0.40
Fe - -
Mo - 5.00
Co - 8.00

Marage 300 - Detail

Steel, Maraging, Bars, Forgings, Tubing, and Rings 18.5Ni - 9.0Co - 4.9Mo - 0.65Ti - 0.10Al Consumable Electrode Vacuum Melted, Annealed

Mechanical properties of grade Marage 300 SAE AMS 6514H (2012)

Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
346 (≥) 316 (≥) 21 11 34 Solution and Aging, Annealing, Ausaging, Q+T,etc 321

Physical properties of grade Marage 300 SAE AMS 6514H (2012)

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
791 (≥) 532 (≥) 43 21 11 Solution and Aging, Annealing, Ausaging, Q+T,etc 311
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
388 888 631