SS 2562 Special Alloy

Chemical composition%of the ladle analysis of gradeSS 2562

C(%)Si(%)Mn(%)P(%)S(%)Cr(%)Ni(%)Mo(%)Cu(%)
Max 0.025Max 1.0Max 2.0Max 0.04Max 0.03019.0-21.024.0-26.04.00-5.001.20-2.00
Swedish SS standard stainless steel and heat resistant steel

Mechanical properties of gradeSS 2562

Proof strength
Rp0.2(MPa)
Tensile strength
Rm(MPa)
Impact energy
KV(J)
Elongation at fracture
A(%)
Reduction in cross section on fracture
Z(%)
As-Heat-Treated Condition Brinell hardness(HBW)
149(≥) 791(≥) 44 24 21 Solution and Aging,Annealing,Ausaging,Q+T,etc 222

Physical properties of grade SS 2562

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J/kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
758(≥) 572(≥) 11 33 34 Solution and Aging,Annealing,Ausaging,Q+T,etc 442
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0)N/mm2
Creep rupture strength
(10000h)
(Rp1,0)N/mm2
813 315 928

SS 2562 Range of products

Product type Products Dimension Processes Deliver Status
Plates/Sheets Plates/Sheets 0.08-200mm(T)*W*L Forging,hot rolling and cold rolling Annealed,Solution and Aging,Q+T,ACID-WASHED,Shot Blasting
Steel Bar Round Bar,Flat Bar,Square Bar Φ8-1200mm*L Forging,hot rolling and cold rolling,Cast Black,Rough Turning,Shot Blasting,
Coil/Strip Steel Coil/Steel Strip 0.03-16.0x1200mm Cold-Rolled&Hot-Rolled Annealed,Solution and Aging,Q+T,ACID-WASHED,Shot Blasting
Pipes/Tubes Seamless Pipes/Tubes,Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion,Cold Drawn,Welded Annealed,Solution and Aging,Q+T,ACID-WASHED